TASARIMDAN İMALATA

Plastic Moulding Shrinkage

Plastic Moulding Shrinkage
← Back to Technical Information
Plastic Moulding Shrinkage

s: shrinkage defined relative to the mould dimension; Lp: target part dimension; Lm: mould dimension. One fixed percentage per polymer family is unreliable. Grade, fibre reinforcement, flow direction, packing, mould temperature and measurement timing affect results.

Material / grades (%)ISO 294-4
ABS — Terluran GP-350.4–0.7linear
PA6 — Ultramid B3S0.90 / 0.90parallel / transverse
PC — Makrolon 24050.65parallel to flow; 60×60×2 mm; 500 bar

Values apply to the named commercial grade and test conditions, not to every material in the family. — means no verified value is provided here. Use the manufacturer's data sheet and material certificate.

s = (Lm − Lp) / Lm
Lm = Lp / (1 − s)

Assumed example: Lp = 100 mm, s = 1.5% → Lm = 101.523 mm. This is not a recommended material value. Obtain flow and transverse shrinkage from the grade data sheet and verify through mould trials.

s (%)Lp (mm)Lm (mm)
0.4100100.402
0.5100100.503
0.65100100.654
0.7100100.705
0.9100100.908
1100101.010
1.5100101.523
2100102.041

Dry and conditioned PA values differ. Moisture affects stiffness and dimensions; consider service humidity.

Technical sources